Effect of Sc and Zr on microstructures and mechanical properties of
as-cast Al-Mg-Si-Mn alloys
(School of Materials Science and Engineering, North University of China, Taiyuan 030051, China)
Abstract: Microstructures of as-cast Al-Mg-Si-Mn alloys with and without Sc and Zr were investigated by optical microscopy, scanning electronic microscopy(SEM) and energy dispersion spectrum analysis. Addition of 0.2%−0.4% Sc can refine the grain size and change the growth morphology from dendritic to fine equi-axial crystal. The higher the addition of Sc, the finer the as-cast grain size. The tensile strength is increased by more than 30% with 0.4% Sc. Moreover, an addition of 0.1%−0.2% Zr is able to refine grain size and change the growth morphology from dendritic to equi-axial grain too, but less effective. However, Zr is found to increase the ductility of the cast alloys, and the elongation is increased to 11.97% with 0.2% Zr.
Key words: Al-Mg alloy; Sc; Zr; microstructure; mechanical properties