Iron extraction from lead slag by bath smelting
(1. School of Metallurgy and Environment, Central South University, Changsha 410083, China;
2. Chinese National Engineering Research Centre for Control and Treatment of Heavy Metal Pollution,
Central South University, Changsha 410083, China)
Abstract: A new bath smelting process was proposed to recover iron for solid wastes reduction. 99.79% of iron metallization, 99.61% of iron recovery, pig iron with 93.58% Fe, 0.021% S, 0.11% P, 1.38% C, 0.22% Si, 0.01% Pb and 0.031% Zn were achieved after the wastes were smelted at 1575 °C for 20 min under C/Fe molar ratio of 1.6 and basicity of 1.2. The produced pig iron could be used in steel-making. This study provides a way for recycling iron from smelting slag and hydrometallurgical residue.
Key words: lead slag; iron extraction; bath smelting; pig iron